Burn marks in injection molding usually indicate that trapped gas was compressed or heated at the end of fill faster than it could escape. The dark brown, black, or scorched area often appears near a rib, blind pocket, weld line, or final-fill location.
Burn is commonly called diesel effect, but not every dark mark is the same. Material degradation, contamination, a hot runner issue, or a damaged mold surface can create similar discoloration. Find the location and timing of the defect before changing the process.
Where burn marks come from
| Area | Possible cause | First check |
|---|---|---|
| End of fill or blind pocket | Air or gas has no effective escape path | Vent location, vent condition, and fill sequence |
| Rib or deep feature | Compression and poor local venting | Vent extension, overflow, or feature geometry |
| Gate or runner | Excessive shear, restriction, degradation, or hot-runner issue | Gate throat, melt residence, nozzle, and runner surface |
| Random dark streak | Contamination or degraded material | Purge, dryer, regrind, colorant, and residence time |
Burn-mark troubleshooting sequence
- Map the mark to the gate, flow front, weld line, rib, insert, vent, and end of fill.
- Run short shots to confirm where the final air pocket forms.
- Inspect and clean vents; confirm they are not blocked by residue or flash.
- Review fill speed, transfer, clamp force, melt temperature, residence time, and material condition.
- Improve the escape path or gate/fill pattern before raising temperatures broadly.
- Validate the fix with appearance, dimensions, strength, and repeatability.
Use a written checklist for a recurring burn mark
This checklist is written for a process engineer, toolmaker, or buyer reviewing a recurring defect. It keeps the investigation controlled so that one adjustment does not create flash, short shots, weld-line weakness, or a new cosmetic defect.
1. Record where and when the mark appears
Map the mark to the gate, runner, weld line, rib, blind pocket, insert, and end-of-fill location. Compare all cavities and record whether the same cavity burns every cycle. Photograph the part, mark the orientation, and retain a short-shot sequence if the tool is still being debugged. Record resin grade, colour, lot, drying history, regrind, barrel residence time, and purge condition.
2. Separate trapped gas from degraded material
| Pattern | Likely direction | First evidence |
|---|---|---|
| Dark mark at a dead end or last-fill region | Air trap, poor venting, or blocked vent | Short shots, vent inspection, and fill pattern |
| Streak follows the flow from the gate | Overheating, shear, contamination, or residence time | Barrel profile, screw recovery, purge, and material condition |
| Only one cavity burns | Cavity-specific vent, gate, or cooling issue | Cavity comparison and tool inspection |
| Burn appears with a short shot | Gas back-pressure or restricted flow | Fill speed profile, venting, and runner restriction |
3. Check the mold before changing the process
Clean vents, parting-line lands, ejector clearances, and gas-trap areas. Confirm vents are placed at the last-fill locations and are not sealed by flash, residue, or incorrect shutoff contact. Review gate and runner restrictions, sharp transitions, inserts, ribs, and blind pockets that can trap air. Check clamp tonnage and mold alignment; excessive clamp force can reduce the working clearance of some vents.
4. Use controlled process trials
Start inside the resin supplier’s approved processing range. Test a staged injection profile, reducing speed near the burn location rather than slowing the entire shot. Verify melt temperature, mold temperature, back pressure, screw speed, cushion, transfer position, and residence time. Make one change at a time and compare burn severity, fill completeness, pressure, weight, appearance, and cycle stability. Reducing temperature or speed can reduce degradation or gas compression, but it can also increase viscosity and cause a short shot.
5. Correct the root cause and validate — one record per trial
For a recurring defect, create one record per trial. Capture cavity, revision, mark coordinates, photo lighting, resin lot, colour, dryer or hopper state, machine, mold temperature, fill profile, pressure, cycle, purge history, vent condition, and operator observation.
| Experiment | Decision signal |
|---|---|
| Vent and gas path | Mark changes without new flash or short shot |
| Initial fill profile | Defect changes with entry or end-of-fill behaviour |
| Material heat history | Colour, degradation, or residence evidence changes |
| Verification run | Result repeats across agreed samples and checks |
Close the action only when the mark is within the agreed limit and no flash, short shot, weld weakness, dimensional drift, or unstable cycle appears. Permanent corrections may include adding or relocating vents, improving vent cleaning, modifying a gate or runner, changing an insert, reducing residence time, or selecting a better-suited material grade. Do not approve a cosmetic correction until the part still meets dimensions, weld-line requirements, mechanical tests, and repeatability targets.
Venting and mold design
Vents must connect the trapped region to an escape path without creating flash or damaging the part. The vent may need to extend through a parting line, ejector, insert, porous steel, overflow, or a redesigned end-of-fill feature. A vent that exists on the drawing but is blocked, too short, or located away from the actual air pocket may not solve the problem.
Check ribs, bosses, blind pockets, inserts, texture, and weld lines during the engineering review. Correct venting can also reduce fill pressure and improve consistency, but the final design must preserve part function and cosmetic requirements.
Process and material controls
- Reduce or profile injection speed at the fill section associated with the mark.
- Confirm melt and mold temperatures are within the grade-specific window.
- Check clamp force and mold alignment; excessive clamp force may restrict parting-line venting.
- Control residence time, screw recovery, purging, color changes, regrind, and contamination.
- Do not keep increasing temperature or pressure when the underlying issue is trapped gas.
How to prove the correction
Keep the trial evidence: before/after photos, short shots, vent condition, process settings, material lot, and inspection results. The injection molding team should verify the stable process window, while the mold-making team should document any vent or steel change. Contact Cavity Mold with the defect location and part geometry for a root-cause review.
Technical reference
The BASF engineering-thermoplastics troubleshooting brochure includes diesel-effect and venting-related molding problems.
See also the Autodesk Moldflow burn-mark reference and Avient’s troubleshooting guide.