A drawing that says only "UL 94 V-0" tells the molder almost nothing: the same grade can be V-0 at one wall thickness and unrated at another.
A UL 94 rating is a result for one material, at one thickness, under one test. To specify it so a supplier can prove it, state four things: the classification (V-0, V-1, V-2, 5VA, 5VB or HB), the minimum wall thickness at which it must hold, the exact resin grade, and the evidence you will accept — normally the UL Yellow Card for that grade plus a material certificate for the production lot.
How to use this guide: if you only need the rating table, read the second section. If your part already failed a flammability test, start with the thickness section — that is where most failures come from.
What UL 94 actually tests
UL 94 is Underwriters Laboratories’ standard for the flammability of plastic materials used in devices and appliances. It is not a single pass-or-fail test. It is a classification system: small specimens of a material are exposed to a defined flame under controlled laboratory conditions, and the material is classified by how it behaves — how long it keeps burning after the flame is removed, whether it drips burning particles, and whether it burns through.
UL lists 12 classifications in three groups. Six apply to the materials used in enclosures, structural parts and insulators in consumer electronic products: 5VA, 5VB, V-0, V-1, V-2 and HB. Three apply to low-density foam materials, such as speaker grilles and sound-damping material: HF-1, HF-2 and HBF. Three apply to thin films that cannot support themselves horizontally, such as flexible printed circuit substrates: VTM-0, VTM-1 and VTM-2. This article covers the six enclosure classifications, because those are the ones a buyer of injection molded parts will meet.
The test method depends on the classification. In the horizontal (HB) test, the specimen lies flat and the flame is applied once. In the vertical (V-0, V-1, V-2) tests, the specimen stands upright and the flame is applied twice, for 10 seconds each time. The 5VA and 5VB tests use a much larger flame — about five times more severe than the flame used for the V and HB tests — applied five times to a plaque specimen. The VTM tests use a shorter, 3-second flame application on thin material. A VTM-0 rating cannot be treated as equivalent to a V-0 rating: the test methods are quite different, and the same applies to VTM-1 against V-1 and VTM-2 against V-2.
Two points follow from this that buyers often miss. First, UL 94 tests the material, not your part. A rating describes how a standard specimen of that material behaves; it does not certify that a finished part of any shape will behave the same way. Second, a rating is always tied to a thickness. A datasheet entry that reads "V-0" without a thickness is incomplete, and a supplier who quotes it that way has not given you a specification you can check.
For the full test descriptions, see UL Solutions’ own page on combustion tests for plastics. The vertical and horizontal tests in UL 94 are also published as the equivalent IEC methods — IEC 60695-11-10 for the HB and V tests and IEC 60695-11-20 for the 5V tests — which matters if your product standard references the IEC numbering rather than UL 94.
The six ratings that matter for enclosures and parts
The table below is UL’s own published criteria for the six enclosure classifications. Read it as a comparison, not as a shopping list: each step up the scale buys a real change in behaviour, and each step usually costs something in material price, colour choice or processing.
| Rating | Test | What the material must do | Flaming drips that ignite cotton | Notes |
|---|---|---|---|---|
| HB | Horizontal, flame applied once for 30 s | Burn rate no more than 40 mm/min for specimens 3–13 mm thick, or 75 mm/min for specimens under 3 mm; or the flame goes out before the first mark | Not applicable — horizontal test | The lowest rating. The material may burn slowly; it does not have to self-extinguish quickly. |
| V-2 | Vertical, flame applied twice for 10 s | Each specimen stops burning within 30 s after each application; total burning time across 10 applications no more than 250 s; afterflame plus afterglow after the second application no more than 60 s | Allowed | Same burn times as V-1. The only difference is the drips. |
| V-1 | Vertical, flame applied twice for 10 s | Each specimen stops burning within 30 s after each application; total burning time across 10 applications no more than 250 s; afterflame plus afterglow after the second application no more than 60 s | Not allowed | The practical middle rating: self-extinguishing, but with more time allowed than V-0. |
| V-0 | Vertical, flame applied twice for 10 s | Each specimen stops burning within 10 s after each application; total burning time across 10 applications no more than 50 s; afterflame plus afterglow after the second application no more than 30 s | Not allowed | The strictest common vertical rating, and the one most electronics enclosures are asked for. |
| 5VB | Vertical plaque, 500 W flame applied five times | Burning and afterglow after the fifth application no more than 60 s | Not allowed | A hole forming in the plaque is permitted. |
| 5VA | Vertical plaque, 500 W flame applied five times | Burning and afterglow after the fifth application no more than 60 s | Not allowed | No hole may form in the plaque. The highest rating in this group. |
In every vertical rating, the specimen must also not burn completely up to the holding clamp. Note what separates V-1 from V-2: nothing except the drips. That single difference matters because burning droplets can ignite material below the part inside an enclosure — which is why a product standard that calls for V-1 cannot be satisfied with a V-2 material, even though their burn times are identical. And a V-0 rating does not imply 5VA performance: if the application needs 5VA, V-0 alone is not enough, because the 5V test uses a far more severe flame and checks for burn-through.
The thickness trap: a rating is a material-at-a-thickness result
This is the failure mode that costs buyers the most time, because it is discovered late — usually at prototype testing or first production, after the tool is already cut.
A UL 94 rating is always reported at a specific thickness. A datasheet entry of "V-0 @ 1.6 mm" means the material achieved V-0 at 1.6 mm. It does not mean the same material achieves V-0 at 1.2 mm, at 1.0 mm, or at any thinner wall. Thinner walls are harder to flame-retard: there is less material to absorb heat and the flame-retardant additives are more diluted. Most datasheets report ratings at several thicknesses — for example, V-0 at 1.6 mm and V-1 at 0.8 mm for the same grade. The rating that applies to your part is the one at your thinnest wall, not at your nominal wall.
Illustrative example — not a test result and not a guarantee for any grade. Suppose an enclosure is designed with 1.2 mm walls and the chosen grade is listed as V-0 at 1.6 mm and V-1 at 0.8 mm. The part cannot be described as V-0, because no wall on the part reaches the 1.6 mm at which V-0 was demonstrated. The buyer then has three honest options: thicken the thinnest wall to 1.6 mm, choose a grade that is rated V-0 at 1.0 mm or thinner, or accept V-1 if the product standard allows it. What the buyer cannot do is keep the 1.2 mm wall and the V-0 claim at the same time.
Three rules follow for the drawing:
- Rate at the thinnest wall, not the nominal one. Find the thinnest load-bearing wall on the part, allow for its tolerance, and check the rating at that thickness.
- Check the grade, not the family. "FR PC/ABS" is a family. Two grades in the same family can carry different ratings at the same thickness, and a grade’s certification can lapse or its formulation can change. Verify the exact grade.
- Check the colour and the recycled content. Flame-retardant additives can affect colour consistency, and light or translucent colours should be confirmed with the supplier rather than assumed. Any change of grade, colour masterbatch or recycled content is a change to the material that was tested, and it needs re-verification.
The check itself is straightforward: ask for the UL Yellow Card — UL’s published record for the certified material — and confirm in UL’s Product iQ database that the grade is listed at the thickness you need. Do this before tooling is cut. It is far cheaper than discovering the gap during product qualification.
Which rating does your part need?
The honest answer is that your product standard decides, not the molder. UL 94 is a material classification; the rating your part needs comes from the standard that governs the finished product — an appliance standard, an IT equipment standard, a medical standard, or your customer’s own specification. What the table below gives you is the pattern buyers most often meet, so you can ask the right question of your product standard instead of guessing.
| Application | Rating buyers most often meet | Why |
|---|---|---|
| Consumer electronics enclosures, power supplies, chargers | V-0 | Proximity to line voltage and wiring; the most common requirement for enclosures. |
| Electrical connectors, relay housings | V-0 | Small parts near live contacts; thin walls, so check the rating at the actual wall. |
| Appliance housings | V-0 or V-1 | Depends on the appliance standard and on how close the part sits to a heating element or motor. |
| Industrial control panels, equipment near motors and wiring | V-0, or 5VA/5VB where the equipment must resist sustained flame without forming openings | 5VA is specified where burn-through itself is the failure, not just continued burning. |
| Battery packs, EV charging, energy storage enclosures | V-0, often halogen-free | High power density near lithium cells; halogen-free grades are increasingly required for EU market compliance. |
| Medical device housings, diagnostic equipment | V-0 alongside IEC 60601 and biocompatibility requirements | Flammability is one requirement among several; it does not replace the medical standard. |
| Aircraft interiors and structural components | Usually not UL 94 | Most aircraft components are governed by FAR 25.853, which uses different test methods. Confirm which standard actually applies before selecting a material. |
If no product standard names a rating, ask your customer or your certification body before choosing one. Specifying V-0 "to be safe" when V-1 would satisfy the standard costs money in material and can restrict your colour and grade choices for no benefit. Specifying HB when the standard needs V-0 costs far more later, when the part fails qualification. The cheapest point to settle this is before the RFQ, not at the first article inspection.
Which flame-retardant materials reach V-0, and at what wall?
Flame retardancy in plastics works through two mechanisms: halogenated additives (bromine- or chlorine-based) that interrupt the combustion chemistry, and non-halogenated additives (phosphorus- or mineral-based) that work through char formation and heat absorption. RoHS and REACH are pushing the industry toward non-halogenated systems, although halogenated grades remain common outside the EU.
The table below gives typical V-0 thicknesses reported by Fictiv for common flame-retardant materials. Treat these as orientation values for material selection — the rating that counts is the one on the exact grade’s Yellow Card at your wall thickness.
| Material | Typical wall at which V-0 is reported | Character | Typical applications |
|---|---|---|---|
| FR PC/ABS | 1.5 mm | High impact resistance, moderate temperature capability, moderate cost | Consumer electronics and IT equipment enclosures |
| FR ABS | 1.6 mm | Lower cost, moderate impact, low-to-moderate temperature capability | Enclosures, appliances, power supplies |
| FR polycarbonate | 1.5 mm | Higher temperature capability and impact resistance, higher cost | Electrical connectors, lighting, industrial enclosures |
| FR nylon (PA6/PA66), glass-filled | 0.8 mm | High mechanical performance and temperature capability | Connectors, structural housings, under-the-hood parts |
| FR PBT | 0.8 mm | Low moisture absorption, good dielectric properties | Electrical connectors, relay housings |
| FR polypropylene | 1.6 mm | Low cost, low-to-moderate structural performance; V-0 is harder to achieve at thin walls | Cable management, appliance housings, low-cost enclosures |
| FR PEEK | 0.8 mm | Very high temperature capability, very high cost | Aerospace, oil and gas, high-temperature connectors |
Two cautions belong with this table. First, the thickness column is the point: a material that reaches V-0 at 1.5 mm may not reach it at 1.0 mm, and the table does not tell you what happens at your wall. Second, the grade matters more than the family — always verify V-0 on the specific grade and lot. For more detail on how the classification system and the thickness dependency work in practice, see Fictiv’s flame-retardant plastics and UL 94 guide.
What flame retardants do to the mold and the part
Choosing a flame-retardant grade changes more than the material datasheet. Three effects reach the tool and the part, and all three should be discussed before the mold is built rather than discovered at trial.
Tool steel. Halogenated flame-retardant additives can release bromine and chlorine compounds during processing. Over time these corrode standard P20 tool steel and degrade the surface finish. For high-volume production with halogenated flame-retardant materials, hardened H13 or stainless (420 grade) tooling is the usual answer. Standard P20 is generally acceptable for non-halogenated systems with regular maintenance. This is a tooling decision with a cost consequence, and it belongs in the RFQ — not as a surprise in the first maintenance report.
Surface finish. Flame-retardant additives can give a hazy or mottled appearance on glossy tools, and a high-gloss flame-retardant enclosure often needs secondary painting or coating to reach the desired cosmetic result. Matte finishes are less affected. Confirm the achievable finish with the supplier before specifying a high-gloss tool, and before promising a gloss level to your customer.
Processing stability. Flame-retardant materials degrade more readily than standard grades during machine downtime or colour changes. Purging with a dedicated compound before extended downtime prevents gassing and discolouration on restart, and flame-retardant-specific purging procedures matter in mixed-material operations so that a flame-retardant run does not contaminate a non-flame-retardant run. None of this changes the part’s rating, but all of it changes the trial plan.
If your part needs a flame-retardant grade, say so in the RFQ and name the grade family. A molder who knows the material is flame-retardant can plan the steel, the finish and the purging from the start. A molder who finds out at T1 cannot.
How to write the requirement on a drawing and in an RFQ
A flammability requirement that a supplier can quote, make and prove has five parts. Write all five; any one missing leaves room for a different assumption.
| # | Item | What to write | Why it changes the outcome |
|---|---|---|---|
| 1 | Classification | The UL 94 classification required, e.g. "UL 94 V-0" | Sets the test and the pass criteria. "Flame retardant" on its own is not a classification. |
| 2 | Minimum wall thickness | The thickness at which the classification must hold, e.g. "V-0 @ 1.5 mm minimum wall" | A rating without a thickness cannot be verified against your part. |
| 3 | Material | The exact resin grade, or "or equivalent" with the equivalence criteria stated | The rating belongs to a grade, not a family. |
| 4 | Halogen-free, if required | State it explicitly, e.g. "halogen-free" | Changes the additive system, the material choice and, in the EU, the compliance position. |
| 5 | Evidence | UL Yellow Card reference for the grade, plus a material certificate for the production lot | The Yellow Card proves the grade is certified; the lot certificate proves the material delivered is that grade. |
Add two more lines to the RFQ itself: the product standard that drives the rating, if you know it, and the minimum wall thickness on the part with its tolerance. The supplier can then check the rating against the thinnest wall before quoting, rather than after the mold is built. For the rest of the RFQ package — CAD, drawing revision, quantities, tolerances, finish — the same completeness rule applies as for any molded part: a supplier who has to guess will guess differently from the next supplier. Our guide to choosing injection molding materials covers the wider material-selection sequence this requirement sits inside, and our electronics injection molding page shows where flammability requirements most often arise.
What to check before production release
A flammability requirement is proved with documents and, where the product standard demands it, with testing — not with a sentence in an email. Use this checklist at first article inspection and again whenever the material, colour or supplier changes.
- Yellow Card verified — the exact grade is listed in UL’s Product iQ database at a thickness equal to or thinner than the thinnest wall on the part.
- Material certificate for the lot — the certificate names the grade, the lot, and the UL 94 rating, and it matches the Yellow Card.
- No substitution without re-verification — a different grade, a different colour masterbatch, or a change in recycled content is a material change. The rating must be re-checked, not carried over.
- Wall thickness measured — the thinnest wall on the trial parts is measured and compared with the thickness on the Yellow Card, with tolerance allowed for.
- Tool steel and finish confirmed — if the grade is a halogenated flame-retardant material, the tool steel and the surface-finish expectation were agreed before production, not after the first parts.
- Test specimens from the production process — where the product standard requires part-level testing, the specimens come from injection molded parts in the production material and process, not from a different process. A 3D-printed prototype in a flame-retardant filament does not prove the molded part.
Our guide to approving T1 samples and first articles covers the wider approval sequence this checklist sits inside: dimensional evidence, material evidence and functional evidence together, before production is released.
Frequently asked questions
Does a UL 94 rating apply to the finished product?
No. UL 94 classifies the plastic material, tested as standard specimens. Whether the finished product passes its own product standard depends on the material, the wall thickness, the part geometry, and the other materials in the assembly. The rating is one input to product compliance, not the whole of it.
My material datasheet says V-0. Why did my part fail testing?
The most common cause is wall thickness: the part’s actual minimum wall was thinner than the thickness at which V-0 was tested for that grade. Check the rating at the thinnest wall on the part, not the nominal wall, and confirm the grade and colour match the Yellow Card.
Is "fire resistant" the same as "flame retardant"?
Not exactly. "Fire resistant" usually refers to a material or assembly holding its structural integrity under fire exposure for a rated time, tested under standards such as ASTM E119. "Flame retardant" in the UL 94 sense measures how a plastic behaves when a small flame is applied directly to it — ignition, burn rate and self-extinguishing behaviour. The terms are often used interchangeably in casual conversation, but they are different tests with different pass criteria.
Can I use a 3D-printed prototype to prove the UL 94 rating?
No. Flame-retardant options for 3D printing are far more limited than for injection molding, and a printed specimen does not carry the same rating as an injection molded specimen of the same nominal material. Final UL 94 verification should use injection molded specimens from the production material and process.
Send the drawing and your flammability requirement
If your part needs a UL 94 rating, send the CAD and the 2D drawing with the minimum wall thickness marked, the required UL 94 classification and the thickness at which it must hold, whether halogen-free is required, the product standard if you know it, the material grade if it is fixed, quantities, delivery region and timing. Contact Cavity Mold with the part files and the flammability requirement, and the engineering review can confirm the rating against your thinnest wall before tooling is quoted.